§ WPS template

AWS D1.1:2025 GMAW WPS for ASTM A992

How to draft an AWS D1.1:2025 Welding Procedure Specification for Gas Metal Arc Welding (GMAW) on ASTM A992 Wide-Flange Structural Steel. Recommended filler: ER70S-6. Below: process notes, base metal properties, prequalification path, typical parameters, and which essential variables to watch.

About GMAW (Gas Metal Arc Welding)

Solid-wire continuous-feed process with external shielding gas (typically 75/25 Ar/CO₂ or 90/10 Ar/CO₂). Constant voltage (CV) output and a fixed wire feed speed give a stable arc. Transfer mode (short-circuit, globular, spray, pulsed) is selected by voltage + current combination. Note: A5.36 was dropped from the AWS D1.1:2025 Table 6.6 allowed-spec list for GMAW.

Process family: semi-auto. Suited to: shop fabrication of structural members, high-deposition shop welds, and similar work.

About ASTM A992

The current standard for wide-flange (W) shapes in US steel construction. Replaced A36 as the default for W-shapes circa 2003. Yield range controlled (50-65 ksi) for predictable seismic performance.

AWS D1.1:2025 Group (Table 5.6)
Group II
Yield (ksi)
50–65 (50 min)
Tensile (ksi)
65 min
Weldability
good

Prequalification path

ASTM A992 (Group II) is on the prequalified base metals list for GMAW per AWS D1.1:2025 Clause 5. A written WPS is still mandatory but no PQR test is required as long as every Clause 5 essential variable (joint geometry, filler, preheat, current/polarity, etc.) is met.

Preheat: Same as A572 Grade 50: 50°F to 3/4 in; 150°F from 3/4 in to 1-1/2 in; 225°F above (low-hydrogen).

Typical parameters

Starting points only. Verify against electrode manufacturer data and your PQR.

FillerER70S-6
Amperage150–280 A (0.045 in wire)
Voltage22–28 V (spray transfer)
Travel speed10–25 ipm
Position(s) typically qualifiedAll positions (1G–4G); 5G/6G for pipe per Clause 10

Essential variables to watch (AWS D1.1:2025 Table 6.6)

If your shop is working from a PQR, these are the GMAW-specific changes that require requalification per Table 6.6. The rule engine flags every one of them with the row number, clause reference, and the actual delta.

  • Shielding gas composition (any change)
  • Voltage > 7% change
  • Amperage > 10% change
  • Wire diameter increase
  • Transfer mode change (short-circuit ↔ spray ↔ pulsed)
  • CV ↔ CC output change

Where GMAW on ASTM A992 fits

  • Wide-flange columns and beams (W-shapes)
  • Special and moment-frame seismic applications
  • Composite beams
  • AISC 360 / 341 conforming structures

Start now

Draft this WPS in the next 2 minutes.

Create a free account and the editor opens with this GMAW + ASTM A992 setup preselected. Free drafts are rules-checked; the 14-day trial adds AI narrative with inline AWS D1.1:2025 citations. Export as a PDF, your CWI signs.

Related WPS templates

FAQ

Does AWS D1.1:2025 prequalify GMAW on ASTM A992?

Yes — ASTM A992 is on the Clause 5 prequalified base metals list and GMAW is a Clause 5 prequalified process. You still need a written WPS but no PQR.

What filler is recommended for GMAW on ASTM A992?

ER70S-6. Verify against your project specification and the consumable manufacturer's data sheet. Filler classification change is a Table 6.6 essential variable.

What preheat does ASTM A992 need?

Same as A572 Grade 50: 50°F to 3/4 in; 150°F from 3/4 in to 1-1/2 in; 225°F above (low-hydrogen).