§ WPS template
AWS D1.1:2025 FCAW WPS for ASTM A36
How to draft an AWS D1.1:2025 Welding Procedure Specification for Flux-Cored Arc Welding (FCAW) on ASTM A36 Carbon Structural Steel. Recommended filler: E71T-1. Below: process notes, base metal properties, prequalification path, typical parameters, and which essential variables to watch.
About FCAW (Flux-Cored Arc Welding)
Tubular flux-cored electrode with either external gas shielding (FCAW-G) or self-shielding (FCAW-S). Higher deposition rates than SMAW or GMAW. Slag covering the bead helps stability and out-of-position performance. Note: A5.36 was dropped from the 2025 Table 6.6 allowed-spec list for FCAW.
Process family: semi-auto. Suited to: high-deposition shop and field welding, out-of-position welding (fcaw-s with self-shield), and similar work.
About ASTM A36
The default structural carbon steel for non-critical applications. Carbon content typically 0.25-0.29%, low carbon equivalent, excellent weldability with both low-hydrogen and non-low-hydrogen consumables. Plate, bar, and shapes.
- AWS D1.1:2025 Group (Table 5.6)
- Group I to 3/4 in, II above
- Yield (ksi)
- 36
- Tensile (ksi)
- 58–80
- Weldability
- excellent
Prequalification path
ASTM A36 (Group I to 3/4 in, II above) is on the prequalified base metals list for FCAW per AWS D1.1:2025 Clause 5. A written WPS is still mandatory but no PQR test is required as long as every Clause 5 essential variable (joint geometry, filler, preheat, current/polarity, etc.) is met.
Preheat: No preheat required for thicknesses ≤ 3/4 in at typical heat inputs; 50°F minimum below 3/4 in, 150°F at 1-1/2 in and above per Table 5.7.
Typical parameters
Starting points only. Verify against electrode manufacturer data and your PQR.
| Filler | E71T-1 |
| Amperage | 180–280 A (0.045 in wire) |
| Voltage | 24–28 V |
| Travel speed | 8–18 ipm |
| Position(s) typically qualified | All positions (1G–4G); 5G/6G for pipe per Clause 10 |
Essential variables to watch (AWS D1.1:2025 Table 6.6)
If your shop is working from a PQR, these are the FCAW-specific changes that require requalification per Table 6.6. The rule engine flags every one of them with the row number, clause reference, and the actual delta.
- Filler classification change
- Shielding gas composition (FCAW-G)
- Voltage > 7% change
- Amperage > 10% change
- Travel speed > 25% change
Where FCAW on ASTM A36 fits
- Light to medium structural framing
- Miscellaneous and ornamental steel
- Base plates and gussets
- Non-load-critical components
Start now
Draft this WPS in the next 2 minutes.
Create a free account and the editor opens with this FCAW + ASTM A36 setup preselected. Free drafts are rules-checked; the 14-day trial adds AI narrative with inline AWS D1.1:2025 citations. Export as a PDF, your CWI signs.
Related WPS templates
FAQ
Does AWS D1.1:2025 prequalify FCAW on ASTM A36?
Yes — ASTM A36 is on the Clause 5 prequalified base metals list and FCAW is a Clause 5 prequalified process. You still need a written WPS but no PQR.
What filler is recommended for FCAW on ASTM A36?
E71T-1. Verify against your project specification and the consumable manufacturer's data sheet. Filler classification change is a Table 6.6 essential variable.
What preheat does ASTM A36 need?
No preheat required for thicknesses ≤ 3/4 in at typical heat inputs; 50°F minimum below 3/4 in, 150°F at 1-1/2 in and above per Table 5.7.