8 min read

CJP Groove Weld CWI Inspection: Step-by-Step Protocol

A structured CWI inspection protocol for complete-joint-penetration groove welds from pre-fit-up through final NDE acceptance — AWS D1.1:2025, organized around QC hold points.

New to procedures? Start with WPS welding: what a welding procedure specification is, with a filled-in example.

A complete-joint-penetration groove weld is structurally the most demanding weld type in a structural steel fabrication program. When CJP welds carry tension loads, fatigue loads, or seismic demand, they represent a failure point that cannot be recovered without full excavation and re-welding. That's why a structured, step-by-step CWI inspection protocol — not a vague "inspect before and after" policy — is the standard of care under AWS D1.1:2025.

This article walks through the full inspection sequence from initial joint assembly to NDE acceptance. Use it to build or audit your internal QC plan.

Rule library based on AWS D1.1:2025; verify against your governing edition — the AHJ or contract may specify 2020 or an earlier revision.

Why a Structured Protocol Matters

Ad hoc inspection — where the CWI checks what's convenient or what the welder flags as ready — produces gaps. The root pass goes uninspected because the shop supervisor didn't call a hold. The preheat wasn't measured at the right location. The backing bar was removed before the CWI saw the root side. Each gap is a potential undetected defect.

A structured protocol converts the code requirements into a checklist with clear sequencing and mandatory stops. The ITP (Inspection and Test Plan) hold/witness/review point system is the contractual version of this; the protocol described here is the technical foundation that the ITP should be built on.

For general ITP structure and hold point classification, see the article on structural welding ITP hold and witness points.

Phase 1: Pre-Fit-Up Verification

Before any joint assembly, the CWI verifies:

Base metal identification: Mill test reports must be on file and traceable to the material in the joint. Verify the heat number or lot against the CMTR. This is especially critical for materials with CVN requirements, where the steel's chemical composition affects PQR applicability. See the CMTR verification guide for the traceability chain.

WPS review: Confirm the WPS covers the joint — process, position, base metal, filler metal, thickness range, backing condition. Verify the WPS is current-revision and that any recent essential variable changes have been evaluated. The WPS must be physically available to the welder at the work station, not just on file in the QC office.

Welder qualification check: Confirm the welder's WPQ is current and covers the process, position, and thickness being welded. For CJP groove welds in structural connections, most shops require 3G + 4G qualification, which covers all positions. Verify continuity — if the welder has not used this process for more than 6 months, they require requalification before proceeding.

Filler metal verification: Check that the filler metal in use matches the WPS filler metal classification. Inspect electrode storage conditions (low-hydrogen SMAW and FCAW-S electrodes require oven storage; FCAW-G wire requires dry storage). Verify H-designation compliance if the WPS specifies a diffusible hydrogen limit.

Phase 2: Joint Fit-Up Inspection

This is the first mandatory hold point. The joint must be inspected and accepted before welding begins.

Root opening and root face: Measure root opening at multiple points along the joint. For prequalified joints, compare to the dimensional tolerances in the applicable Clause 5 joint designation. For tested WPS joints, verify against the range established in the PQR. Document both minimum and maximum root opening values. A joint that varies outside the qualified range requires correction before welding proceeds.

Groove angle: Measure with a protractor gauge. Under-angle joints compress the root gap; over-angle joints waste filler metal and increase distortion. Both extremes outside the qualified range are nonconforming.

Root face: For joints with a specified root face dimension, verify consistency. Variable root face produces variable penetration depth in the first pass.

Joint alignment and hi-lo: Check the alignment of the members being joined. Excessive hi-lo (mismatch in plate surface elevation across the joint) creates asymmetrical stress concentration at the weld toe. AWS D1.1 imposes hi-lo limits that vary by joint type and loading condition. Use a hi-lo gauge — do not estimate by eye.

Backing bar installation (if applicable): If steel backing is specified, verify the backing bar is the correct grade, is in tight contact with the base metal across the full joint length, and is tacked at the required frequency. Gaps between backing bar and base metal produce lack-of-fusion at the root. For more on backing installation requirements, see the CJP groove pre-weld fit-up checklist.

Cleanliness: Joint surfaces must be free of moisture, oil, mill scale in the root area, paint (unless a welding-through primer is specified on the WPS), and other contaminants. For cold-weather conditions, verify that any surface condensation has been removed and the joint area is at or above the WPS minimum preheat before welding begins.

Phase 3: Preheat Verification

Preheat is a mandatory hold point for materials and thicknesses that require it. The CWI must:

Measure preheat temperature: Use a contact thermocouple, temperature-indicating crayon, or infrared thermometer calibrated for the steel emissivity. Measure at a minimum of 3 inches from the weld joint — not on the weld prep surface itself, where localized torch heating can give a false reading. For thick sections (plates over 1.5 in), allow the heat to soak through the section before measuring the opposite face.

Verify minimum temperature: Compare to the WPS-specified minimum preheat. The minimum is the lowest temperature allowed; welding below it is a WPS deviation and a code nonconformance. For minimum preheat by material group and thickness, AWS D1.1:2025 Table 5.11 provides the prequalified values.

Interpass temperature upper limit: Confirm the interpass temperature capability — thermometers or crayons with the correct maximum temperature range must be on hand before the second pass begins.

Document the ambient temperature, measured preheat, and measurement method and location. This documentation becomes part of the weld traveler.

Phase 4: Root Pass Inspection

The root pass inspection is the single most critical inspection point in a CJP groove weld program. This is a mandatory hold point — no subsequent passes until the CWI accepts the root.

Visual inspection of root pass: After the root pass cools enough to remove slag, the CWI performs a visual inspection of the full root pass face. Look for:

  • Root cracks: transverse or longitudinal cracks at the root toe. These are rejectable and must be ground out and re-welded — not covered over.
  • Incomplete fusion at the root: cold lap, lack of tie-in with the base metal or backing bar. Can be difficult to see definitively by eye; if suspected, require NDE before continuing.
  • Excessive convexity: a root pass that is too convex creates notch conditions at the toes that are difficult to correct with subsequent passes.
  • Burn-through or melt-through: excessive penetration that creates a discontinuous root surface.

For CJP joints without backing that require back gouging before the second side, inspect the root pass before back gouging begins. After back gouging, inspect the excavated channel — confirm the full root pass has been exposed, with no slag entrapment or porosity visible in the groove bottom.

Back gouging verification: The gouged channel must expose sound metal across the full joint length. Visual and MT/PT inspection of the gouged surface before welding the second side is best practice on demand-critical welds.

Phase 5: Fill and Cap Pass Monitoring

The CWI role during fill and cap passes is primarily monitoring, not necessarily a halt point for every pass. The key responsibilities:

Interpass temperature monitoring: At intervals during multi-pass welding, measure and record the interpass temperature. If the preheat/interpass temperature specification includes a maximum (which it does when CVN toughness is specified — see Table 6.8 supplementary essential variables), exceeding the maximum requires the joint to cool before proceeding.

Interpass cleaning: Verify that slag is completely removed between passes. Retained slag that is covered by the next pass creates slag inclusion discontinuities. The CWI does not need to watch every pass, but periodic checks confirm the welder's practice.

Parameter compliance: Spot-check ammeters, voltmeters, and wire speed settings against the WPS. Deviations outside the WPS tolerance must be corrected immediately — not at the end of the shift.

Interpass visual: Watch for cracks, porosity, or undercut developing during fill passes, particularly at restart locations and at joint ends.

Phase 6: Post-Weld Visual Inspection

After welding is complete and the joint has cooled to ambient temperature, the CWI performs the final visual inspection per AWS D1.1:2025 Clause 9 visual acceptance criteria:

  • No cracks: visible or suspected cracks require NDE confirmation and repair before acceptance.
  • Fusion: complete fusion to base metal at both toes and between passes.
  • Weld profile: reinforcement within limits; no overlap; acceptable convexity/concavity.
  • Undercut: at or below the allowable limits for the loading category (statically vs. cyclically loaded).
  • Arc strikes: not acceptable on base metal outside the weld zone on demand-critical welds.
  • Weld size: for welds with minimum size requirements, verify throat or leg size with weld gauges.

For backing bar joints, the steel backing removal requirements must be followed before final visual of the root side.

Phase 7: NDE Inspection

If NDE is specified, the CWI verifies:

  • NDE is performed by qualified personnel (UT technicians to ASNT Level II or equivalent; RT film readers to Level II; MT/PT to Level II)
  • The correct joints are examined at the specified sampling rate
  • Results are documented on forms that identify the joint, examination date, technician, and indication location
  • Rejections are formally reported and repair procedures approved before rework proceeds
  • Re-inspection after repair follows the same acceptance criteria as original inspection

The NDE method selection guide covers when UT vs. RT is appropriate for CJP groove weld types.

Building This Into Your QC Plan

For AISC-certified fabricators, the written quality control plan must address each of these inspection phases with clear hold point vs. witness point designations, documentation requirements, and acceptance criteria references. Auditors look for a plan that reflects the actual complexity of CJP groove weld inspection, not a one-line entry that says "inspect welds per AWS D1.1."

Using a digital WPS and inspection management platform that links the WPS, PQR, welder qualifications, and weld traveler documentation to each joint streamlines the evidence trail from pre-fit-up through NDE — especially on multi-shift shops where the CWI at final inspection may not be the one who signed off on fit-up.

FAQ

Frequently asked.

What are the required CWI hold points for a CJP groove weld under AWS D1.1?
AWS D1.1:2025 requires inspection before welding begins (joint fit-up, WPS review, preheat verification), during welding (root pass, interpass temperature, parameter compliance), and after welding (visual acceptance, backing removal if applicable, and NDE if specified). The specific hold versus witness point designation is set by the project ITP, not the code itself.
Can a CWI inspect a CJP weld root pass after the joint has been closed up?
No. The root pass must be inspected before the next pass covers it. Once the root is buried under subsequent passes, root fusion and cracking cannot be evaluated visually. This is a mandatory hold point in any responsible QC plan — stopping production to verify the root before continuing is non-negotiable.
What visual acceptance criteria apply to a completed CJP groove weld in AWS D1.1:2025?
For statically loaded structures, AWS D1.1:2025 Clause 9 visual acceptance criteria apply: no cracks, complete fusion, undercut not exceeding specified limits, weld reinforcement within profile limits, and no overlap or burn-through. Cyclically loaded structures have more restrictive criteria. The CWI must inspect under adequate lighting at an angle that allows detection of surface-breaking discontinuities.
When must NDE be performed on CJP groove welds?
The NDE requirement is set by the design drawing or project specification, not the base AWS D1.1 code. The code establishes acceptance criteria and test methods; the EOR specifies which joints receive NDE and at what sampling rate. CWI role is to verify NDE is performed by qualified personnel on the correct joints, and that rejections are properly documented and repaired before final sign-off.

More from the blog